摘要
Reoxidation of liquid steel containing Al and Ti by 14%CaO-35%Al2O3-10%MgO-41%SiO2 (in mass%) slag was investigated at 1 823 K with initial Al content of 820 mass ppm and Ti content varied from 100 to 500 mass ppm. It was observed that Al and Ti in the steel were simultaneously oxidized by SiO2 in the slag, and the soluble oxygen was supersaturated during the course, particularly with respect to Al. Based on the experimental results, a new mechanism of the reoxidation reaction was proposed, which involves chemical reactions both at the metal/slag interface and in the bulk metal. Self-dissociation of SiO2 into Si and O at the slag/metal interface was found to play an important role in both supersaturation of oxygen, and subsequent formation of complex oxide inclusions. Formation of inclusions having a two-layer structure where an Al2O3 core was enclosed by complex Al-Ti-O oxide was explained in relation with supersaturation of oxygen in the steel.
引用
收藏
页码:1669 / 1678
页数:10
相关论文
共 16 条
[1]   FactSage thermochemical software and databases [J].
Bale, C ;
Chartrand, P ;
Degterov, SA ;
Eriksson, G ;
Hack, K ;
Ben Mahfoud, R ;
Melançon, J ;
Pelton, AD ;
Petersen, S .
CALPHAD-COMPUTER COUPLING OF PHASE DIAGRAMS AND THERMOCHEMISTRY, 2002, 26 (02) :189-228
[2]   Reoxidation behavior of molten steel in non-killed and Al-killed steels [J].
Goto, H ;
Miyazawa, K .
ISIJ INTERNATIONAL, 1998, 38 (03) :256-259
[3]  
Higuchi Y, 1998, TETSU TO HAGANE, V84, P333
[4]  
Huh W., 1996, ISIJ INT, V36, pS136
[5]   A thermodynamic model for deoxidation equilibria in steel [J].
Jung, IH ;
Decterov, SA ;
Pelton, AD .
METALLURGICAL AND MATERIALS TRANSACTIONS B-PROCESS METALLURGY AND MATERIALS PROCESSING SCIENCE, 2004, 35 (03) :493-507
[6]   REOXIDATION OF ALUMINUM IN LIQUID-IRON WITH CAO-AL2O3-FETO (LESS-THAN-OR-EQUAL-TO-3MASS-PERCENT) SLAGS [J].
LEE, KR ;
SUITO, H .
ISIJ INTERNATIONAL, 1995, 35 (05) :480-487
[7]   LIQUID STEEL TREATMENT IN LADLE WITH NON-OXIDIZING SYNTHETIC SLAG [J].
OKOHIRA, K ;
SATO, N ;
MORI, H .
TRANSACTIONS OF THE IRON AND STEEL INSTITUTE OF JAPAN, 1974, 14 (05) :337-346
[8]   Effect of Al on the evolution of non-metallic inclusions in the Mn-Si-Ti-Mg deoxidized steel during solidification: Experiments and thermodynamic calculations [J].
Park, SC ;
Jung, IH ;
Oh, KS ;
Lee, HG .
ISIJ INTERNATIONAL, 2004, 44 (06) :1016-1023
[9]   KINETICS OF ALUMINUM OXIDATION DURING ARGON INJECTION INTO LIQUID STEEL [J].
PLUSCHKELL, W ;
REDENZ, B ;
SCHURMANN, E .
ARCHIV FUR DAS EISENHUTTENWESEN, 1981, 52 (03) :85-90
[10]   Effect of stirring on oxidation rate of molten steel [J].
Sasai, K ;
Mizukami, Y .
ISIJ INTERNATIONAL, 1996, 36 (04) :388-394